Composite Industrial Grade
PLA-GF

PLA-GF – Glass fiber PLA, 115 °C annealed

PLA-GF: 12 % glass fiber, 50.1 MPa tensile strength, HDT/A 114.7 °C after annealing. An insulating functional material without a chamber system.

Technical Specifications

Base Polymer
High-temperature PLA with 12 % short glass fiber (GF)
Tensile Strength
50.1 MPa (X-Y, ISO 527)
Heat Deflection
114.7 °C (HDT/A, annealed)
UV Resistance
Not UV-stabilized

Typical Applications

  • Functional parts up to ~100 °C after annealing
  • Insulating fixtures in electronics manufacturing
  • Jigs that need to be distinguishable by colour
  • Dimensionally stable large areas – shrinkage 0.05 %

Documents will be provided once a specific material is selected.

Material profile

PLA-GF is a high-temperature PLA with 12 % short glass fiber. What makes it interesting is annealing: as printed, heat deflection is 75.5 °C; after 30 minutes at 100 °C it reaches 114.7 °C (HDT/A, ISO 75). That takes a PLA out of prototyping and into functional use.

The second difference from the carbon variant is electrical: glass fiber insulates. For fixtures in electronics manufacturing that is not a detail but the selection criterion.

Values from the manufacturer datasheet

Propertyas printedannealedTest standard
Tensile strength X-Y50.1 MPa50.2 MPaISO 527
Tensile modulus X-Y3,794 MPa4,207 MPaISO 527
Elongation at break X-Y2.8 %2.3 %ISO 527
Flexural strength X-Y86.4 MPa87.8 MPaISO 178
HDT/A (0.45 MPa)75.5 °C114.7 °CISO 75
HDT (1.8 MPa)59.7 °C84.0 °CISO 75
Vicat148.9 °C148.3 °CISO 306
Density1.337 g/cm³ISO 1183

Annealing therefore changes almost only the temperature figures – strength and stiffness stay much the same. If the part is only loaded at room temperature, the step can be skipped.

Processing

Nozzle 210–230 °C, bed 25–60 °C, no enclosed chamber needed. Pre-drying 6 hours at 60 °C. A hardened nozzle from 0.4 mm is mandatory; glass fiber is just as abrasive as carbon. After printing, annealing follows in a convection oven where required.

Request a Quote