Technical Specifications
Typical Applications
- Large prototypes with a hard weight limit
- Lightweight housings and covers
- Structural parts and housings for unmanned aerial vehicles
- Architectural and design models
- Handling aids and fixtures that are carried all day
Compliance Evidence
Free of hazardous substances (lead, mercury, cadmium, hexavalent chromium, PBB, PBDE) per EU Directive 2011/65/EU. Safe for commercial use in the EU.
Evidence: Product-specific test report to IEC 62321-1/-2/-3-1 for EU 2011/65 incl. (EU) 2015/863 – result: complies.
⚠ Partially documented – SVHC statement available, but no complete REACH conformity declaration on file.
Evidence: Statement in the safety data sheet for the filament: contains no substances from REACH Annexes XIV and XVII and none from the candidate list. Applies to the filament, not to the printed part.
The evidence listed applies to the filament or raw material per manufacturer documentation. Regulatory clearance of the printed final product – particularly for food contact, medical devices, electrical applications or UL-relevant parts – is not automatically included and must be evaluated on a project-specific basis. Technical machine assignment is handled internally.
Material Documents
Material profile
LW-PLA is PLA with a blowing agent. Above a certain nozzle temperature that agent expands, so the material occupies more volume than it carries in mass – and the same part weighs less. To make this work, the material flow is reduced in the slicer: the filament foams just enough for the extruded line to return to its nominal width.
The material solves exactly one problem: parts where weight, not strength, is the hard limit. Large models, covers, flying structures, fixtures somebody holds all day.
Documented figures
The following values come from the manufacturer datasheet for Bambu Lab PLA Aero. It is the datasheet in this material class that reports tensile, flexural and impact figures separately for X-Y and Z – the decisive distinction for FFF parts.
| Property | X-Y | Z | Standard |
|---|---|---|---|
| Tensile strength | 24 ± 2 MPa | 18 ± 3 MPa | ISO 527 |
| Tensile modulus | 1350 ± 250 MPa | 1240 ± 180 MPa | ISO 527 |
| Elongation at break | 2.6 ± 0.7 % | 1.2 ± 0.4 % | ISO 527 |
| Flexural strength | 45 ± 4 MPa | 17 ± 3 MPa | ISO 178 |
| Flexural modulus | 1690 ± 120 MPa | 1410 ± 80 MPa | ISO 178 |
| Charpy impact, unnotched | 28.8 ± 1.3 kJ/m² | 3.1 ± 0.7 kJ/m² | ISO 179 |
| Charpy impact, notched | 8.2 ± 0.7 kJ/m² | – | ISO 179 |
Thermal: HDT/A 48 °C and HDT/B 53 °C (ISO 75), Vicat softening 54 °C (ISO 306), glass transition 55 °C, melting temperature 153 °C (DSC). Filament density is 1.21 g/cm³ (ISO 1183) – explicitly the figure for the filament, not for the foamed part.
What the foaming level does to strength
Lighter is not free. The colorFabb LW-PLA datasheet is the only primary source that measures the same material at two process settings:
| Setting | Tensile strength | Modulus | Elongation at break |
|---|---|---|---|
| 200 °C, 100 % flow (practically unfoamed) | 43 MPa | 3350 MPa | 8.1 % |
| 250 °C, 45 % flow (heavily foamed) | 10 MPa | 860 MPa | 12.8 % |
Between “barely foamed” and “heavily foamed” there is roughly a factor of four in strength. The same datasheet states the process rule: the blowing agent activates at about 230 °C and can increase the relative volume of the PLA up to threefold; reducing flow to 65 % produces lightweight parts. We set the foaming level from the load case, not from what is maximally achievable.
Design notes
- Define the load direction. In Z the flexural strength drops to 17 MPa, about a third of the X-Y figure. Load paths and layer orientation have to match.
- No tight fits. Expansion affects the outer dimensions. Where tenths matter, we sample a first article or machine the surface afterwards.
- Wall thickness over infill. The foam saves weight; stiffness comes from cross-section and geometry. Two extra perimeters do more than raising the infill.
- Keep it out of the heat. HDT/A of 48 °C means no engine bay, no sunlit windowsill, nothing next to a heat source.
- Check fine detail. Lettering, thin ribs and sharp edges blur as the foaming level rises.
Where it fits
Against solid PLA: 40 to 65 MPa tensile strength there, but the full weight. Where strength counts, solid PLA or a tough PLA compound such as PolyMax PLA remains the right choice.
Against foamed TPU: TPU Air uses the same principle but is an elastomer – soft, damping, with a closed outer skin. LW-PLA, once printed, is a stiff, hard foam.
Against fiber-reinforced materials: if you need stiffness at low weight, PLA-CF or one of the fiber-reinforced materials serves better – heavier than LW-PLA, but in a different strength class.
What is not documented
We deliberately do not list a part density as a material figure: neither the Bambu nor the colorFabb datasheet states an achievable part density with a test standard. The widespread claim “up to 65 % lighter” appears on a manufacturer product page, not in a tested datasheet – we treat it as a manufacturer statement and sample the weight on a first article. Also not documented: any UL94 flammability class and any food contact evidence.