Technical Specifications
Typical Applications
- Dimensionally stable display models and design samples
- Fixtures and gauges without thermal load
- Stiff housing parts for indoor use
- Trade show parts and prototypes with a matte carbon look
Documents will be provided once a specific material is selected.
Material profile
PLA-CF is PLA with 8 % short carbon fiber by weight. The fiber changes two things noticeably: parts become stiffer, and the surface turns matte anthracite instead of glossy. What it does not change is the temperature limit – PLA remains PLA.
That marks out the application range clearly: parts that should look and feel dimensionally stable, with no heat or chemistry involved. For tooling aids, trade show builds, inspection fixtures in climate-controlled rooms and design samples, this is exactly right.
Values from the manufacturer datasheet
| Property | Value | Test standard |
|---|---|---|
| Tensile strength X-Y | 28.3 MPa | ISO 527 |
| Tensile strength Z | 12.5 MPa | ISO 527 |
| Tensile modulus X-Y | 2,945 MPa | ISO 527 |
| Flexural strength X-Y | 54.2 MPa | ISO 178 |
| Flexural modulus X-Y | 3,215 MPa | ISO 178 |
| Charpy X-Y | 4.82 kJ/m² | ISO 179 |
| HDT/A (0.45 MPa) | 54.0 °C | ISO 75 |
| HDT (1.8 MPa) | 50.4 °C | ISO 75 |
| Vicat | 64.1 °C | ISO 306 |
| Density | 1.29 g/cm³ | ISO 1183 |
The Z value of 12.5 MPa shows the anisotropy plainly: perpendicular to the layer plane the part carries less than half the load. We therefore always align the main load direction with the X-Y plane.
PLA-CF or PLA-GF?
| PLA-CF | PLA-GF | |
|---|---|---|
| Fiber content | 8 % carbon | 12 % glass |
| Tensile strength X-Y | 28.3 MPa | 50.1 MPa |
| Heat deflection | 54 °C | 75 °C, annealed 115 °C |
| Electrical | slightly dissipative | insulating |
| Colours | anthracite only | nine colours |
If the part will see heat or has to insulate, PLA-GF is the better choice. PLA-CF wins on appearance and price.
Processing
Printing requires a hardened nozzle from 0.4 mm – carbon fiber wears out a brass nozzle within hours. An enclosed chamber is not needed; pre-drying only if the filament has been stored open. Equilibrium water absorption is 0.38 %.